The drawing calls for a hardness in HRC, the measuring room only has a Vickers tester, and the mill certificate of the steel states Brinell. Can these values be converted into each other? Yes, but not with a formula, only with a table, and only within clear limits. Here you learn how conversion works, when you can trust it and where it stops.
Three methods, three different measured quantities
All three methods press an indenter into the workpiece. But each one measures something different.
- Brinell (HBW): A carbide ball is pressed in. The diameter of the indentation gives the area, and the hardness is the test force related to this area. The old symbol HBS for the steel ball no longer exists.
- Vickers (HV): A diamond pyramid leaves a square indentation. You measure the two diagonals, and here too the test force related to the area is what counts. The number after HV stands for the test force. HV10 means about 98 N and is common for steel.
- Rockwell C (HRC): A diamond cone is pressed in with a preliminary force and a test force. What is measured is the permanent indentation depth, not the area. Every 0.002 mm of depth lowers the value by one point.
How deep and how wide an indentation becomes does not depend on hardness alone. It also depends on how much the material work-hardens during indentation and how much it springs back elastically. That is why there is no formula that turns HRC into HV. The relationship comes from comparison measurements on many specimens of one material group. This is why it is called conversion by table rather than calculation.
How to read the conversion table
A conversion table puts equivalent values side by side for one material group. A small excerpt for unalloyed and low-alloy steels already shows the key points. This table does not fit high-alloy tool steels such as cold work or high-speed steels.
| HV10 | HBW | HRC |
|---|---|---|
| 200 | 190 | – |
| 300 | 285 | 29.8 HRC |
| 400 | 380 | 40.8 HRC |
| 500 | 475 | 49.1 HRC |
| 600 | 570 | 55.2 HRC |
| 700 | – | 60.1 HRC |
Two things stand out. For steel, Brinell and Vickers are close together, here HBW is about 5 % lower than HV. The HRC values, on the other hand, do not rise evenly. From 300 to 400 HV, HRC rises by 11 points, from 600 to 700 HV by only 5. So one point of HRC means much more in the hard range than in the soft range.
Interpolating intermediate values
If your measured value lies between two rows, you calculate linearly in between. That is allowed. Calculating beyond the end of the table, i.e. extrapolating, is not.
- x your measured value in the known scale
- x1, x2 the table values below and above
- y1, y2 the corresponding values in the scale you are looking for
- y the converted value
Example
A pressure pad made of the low-alloy steel 100Cr6 has been hardened. The drawing requires 54 … 58 HRC. The Vickers tester measured 610 HV10. The table lists 600 HV with 55.2 HRC and 620 HV with 56.3 HRC.
y = 55.2 + 610 − 600620 − 600 · (56.3 − 55.2) = 55.2 + 0.5 · 1.1 = 55.75 ≈ 55.8 HRC
The value lies well within 54 … 58 HRC. That is enough as a check in production. In the report, however, it is entered as a converted value, for example ≈ 55.8 HRC, converted from 610 HV10. If hardness is an acceptance criterion, the test is done with the method stated on the drawing.
The material group decides
There is a separate table for quenched and tempered steels in the quenched and tempered condition, and it differs noticeably. There, 400 HV corresponds to 395 HBW and 41.5 HRC instead of 380 HBW and 40.8 HRC. If you take the wrong group, you are 15 points off in Brinell.
For austenitic stainless steels, cast iron, aluminium or copper alloys, the steel values do not apply at all. Some of these materials have their own tables, many have no reliable conversion.
Where conversion stops
- Soft steels: Rockwell C is not intended for soft steels, the table only starts at just over 20 HRC. You cannot state an annealed steel with 180 HBW in HRC, that is what Brinell or Rockwell B with a carbide ball (HRBW) are for.
- Very hard steels: The carbide ball is only approved up to 650 HBW. That is why there is no Brinell value for hardened steel with 60 HRC, not even a converted one.
- Surface layers: Case-hardened or nitrided parts get softer towards the inside. At 60 HRC the cone penetrates about 0.08 mm permanently and also senses the core. That is why an HV1 value from a thin nitrided layer cannot be converted to HRC. What counts here is the hardness profile, measured with a low test force.
- Tensile strength: Rm is also listed in the table, but hardness only gives a rough indication of it. As a guide value for unalloyed and low-alloy steel, Rm ≈ 3.2 … 3.3 · HV. This does not replace a tensile test.
Common mistakes
- Using a rule of thumb for HRC: Because the HRC divisions are not even, no fixed factor fits. Always use the table.
- Calculating beyond the end of the table: An HRC value for a structural steel with 150 HV or an HBW value for 62 HRC is invented, not converted.
- Ignoring the material group: Quenched and tempered or not makes a difference at the same HV, in Brinell quickly 10 to 15 points.
- Stating the converted value like a measured value: Without the note “converted from …” nobody knows any more how the value came about.
- Leaving out the test force: The values 610 HV10 and 610 HV1 are not the same, especially on surface layers. The test force belongs to the designation.
Frequently asked questions
Why is HBW almost equal to HV for steel?
Both methods relate the test force to the area of the indentation and therefore give similar numbers. For unalloyed and low-alloy steel, HBW in the table is about 5 % below HV. This is a guide value for this material group, not a general rule.
Where do I find this in the app?
In Gesello, in the Convert hardness module. In the Convert tab you choose the material group, As delivered or Quenched and tempered, and enter a value in HV10, HBW, HRC or Rm. You get the other values with the interpolation steps, the scales in comparison and the conversion table. Outside the table range the app does not convert. In the Read designation tab you decode hardness designations such as 610 HV10 or 58 HRC.
Hardness is closely linked to the choice of cutting values. How to find the spindle speed from the cutting speed is shown in the calculation guide Calculating spindle speed and feed rate. How bolt property classes relate to the tightening torque is explained under Tightening torque for bolts.